346 N. Saunders and A, P. Miodownik contain substantial levels of a, in excellent accord with experimental observation. Keefe et al. (1992) further determined TTT diagrams for both U720 and U720LI, which are shown in Figure 10.47. Decreasing the Cr levels must decrease the cr-solvus and, as the high-temperature part of the TTT diagram asymptotes to the <7-solvus temperature, the two TTT diagrams should have distinct and separate curves. Taking the cr-solvus calculated for U720 and U720LI, it was proposed (Saunders 1995, 1996c) that the TTT diagrams should have the form as shown in Fig. 10.48. 100O wo ■ U720/U720LI (o) 0 U720/U720LI (O free) A U720 (a), U720LI (o free) U720 j-1 I I 111, \ i_I I I 11 I I I_I t I I M ioo iooo Hold time (hours) 10000 Fieure 10 47 TTT diagrams for a formation for U720 and U720H after Keefe et al. (1992). iooo «00 750 700 650 ■ U720/U720L1 (o) _ □ U720/U720LI (o free) A U720(o), U720LI (o free) ^---^LI720 U720U^__ - ^•wi a A X" 1 ......1_1_1_L_J_l_IJjJ_l_ _1_1 1 1 1 n U720LI a. 10 100 1000 Hold time (hours) 10000 Figure 10.48 TTT diagrams for U720 and U720LI based on calculated tr-solvus temperatures. CALPHAD—A Comprehensive Guide 347 10.6.1.2 The effect of Re on TCP formation in Ni-based super alloys. As gas turbine engines are designed and manufactured to work at higher and higher thrust-to-weight ratios, the temperature capability of most components has had to be increased. This has applied particularly to the high-pressure (HP) turbine blades where the development of new alloys has followed lines associated both with the development of microstracture and new chemistries. HP turbine blades are now commonly single-crystal materials where the grain boundaries have been removed by novel casting techniques. HP blades have also seen the development of alloy variants which typically contain Re at levels of between 2 and 6wt%. Because Re is such a heavy element, this relates to a small addition in atomic terms, but the effect on properties such as creep and strength is pronounced. Re also has a profound effect on the temperature at which TCPs are observed, raising this substantially (Darolia et al. 1988, Erickson et al. 1985). The reason for this is not readily understood in terms of a PHACOMP approach (Darolia et al. 1988), and it therefore is interesting to look at how CALPHAD methods can deal with an element like Re. CMSX-4 is a second generation single crystal superalloy and typically has the composition Ni-6.3Cr-9Co-0.6Mo-6W-6.5Ta~3Re-5.6Al-lTi-0.1Hf (in wt%). Figure 10.49 shows a calculated phase % vs temperature plot for this alloy and most aspects of its phase behaviour appear well matched. The high-temperature TCP phase is the R phase, in excellent agreement with the work of Proctor (1992) and its predicted composition is also in good agreement with Proctor (1992), with W and Re in almost equal proportions (~35wt% each). It is clear that the partitioning of Re 100 h- m < a. a j o 600 900 1200 TEMPERATURE CELSIUS 1500 Figure 10.49 Calculated mole % phase vs temperature plot for a CMSX-4 Ni-based superalloy. References are listed on pp. 402-408. 348 N. Saunders and A, P. Miodownik to the R phase is particularly strong and even stronger in a, where levels can reach 45wt%. Although the formation of TCP phases is clearly enhanced because they are so rich in Re, their amounts in the alloy are restricted by the total level of Re, in this case only 3wt%. Therefore, the amounts of a and R never rise to catastrophic levels as was evident in the previous example of U720. This has the corollary that Re-containing single-crystal alloys, such as CMSX-4, may be relatively tolerant to TCP formation even though their temperatures of formation can be high. The sensitivity of TCP formation to Re can be further emphasised by examining what happens to CMSX-4 when the Re level is reduced by \ to 1.5wt% accompanied by a corresponding increase in W level. For this case the solvus temperature falls by some 50°C. A similar exercise of replacing Re with W was performed by Darolia et al, (1988) and their observed variations in the start temperature of TCP formation are in reasonable accord with this. It is also evident that there is a complex interplay between the three main TCP phases, a, R and P, with \i occasionally being observed (Darolia et al. 1988, Proctor 1992, Walston et al. 1996). To examine this more closely, calculations were made for CMSX-4 by alternatively suspending two of the three main TCP phases and calculating the behaviour of the alloy with just one of the phases allowed to form at any one time (Fig. 10.50). The solvus temperatures for R, P and a respectively were calculated as being close to each other at 1045°, 1034° and 1026° respectively, and the R and P phases are particularly close in stability over the whole temperature range. It is clear, therefore, that the interplay between the various TCP phases will be sensitive to the alloy composition and indeed changes in Re, W and Cr levels will cause either a, R or P to become the dominant TCP phase. 700 800 900 1000 TEMPERATURE CELSIUS 1100 Figure 10.50 Calculated mole % phase vs temperature plot for a CMSX-4 Ni-based superalloy with only one TCP phase allowed to form at any one time. CALPHAD—A Comprehensive Guide 10.6.2 Complex precipitation sequences 349 10.6.2.1 7000 series Al-alloys. Probably the most complex type of Al alloys are the 7000 or 7XXX series. These are based on the Al^Cu-Mg-Zn quaternary system and hardening reactions are based on one or more of three phases: (1) tj, which is based on the binary Mg-Zn Laves compound but also exists in Al-Cu-Mg; (2) TLAlCuMgZn, which exists in both the Al-Cu-Mg and Al-Mg-Zn systems; and (3) £_Al2CuMg (as in an AA2024 alloy). In these alloys it is the Zn/Mg ratio which is considered most critical in deciding the type of precipitation reaction which takes place. It should be noted that in practice an alloy such as AA7075 achieves maximum hardness due to the precipitation of the metastable rf phase which is structurally related to rj. Also, both the r_AlCuMgZn and iSLAl2CuMg phases can form similar metastable hardening phases. At present, thermodynamic descriptions for these phases do not exist but, because of the inherent relationship between the metastable and stable forms of the compounds, it is reasonable to expect that the metastable precipitate which forms will be closely related to the respective stable precipitate which predominates in the alloy. Also, a number of important questions connected with processing are directly related to the stable forms; for example, solution temperatures and intermediate heat-treatment temperatures and their formation during non-equilibrium solidification. It is therefore instructive to look at a series of calculations for 7XXX alloys to observe how the calculated diagrams vary as the composition of the alloys is changed. Figures 10.51a-d show the precipitation of the three major hardening phases, t], T and S, as well as £-AlCrMnMg and Mg2Si, for a series of high-strength 7000 series alloys with Zn:Mg ratios as given in Table 10.1. For simplicity, other phases which may appear, such as Al6Mn, a, etc., have not been included. AA7049 represents the highest Zn:Mg ratio and also gives one of the highest values for the total percentage (Zn+Mg) total. In this case the hardening phase is almost completely r? and its level rises to a maximum of 6% in molar units. As the Zn:Mg ratio is reduced from 3.1 to 2.7 in the AA7050 alloy the competition between fand r) is still won easily by rj but, due to the high levels of Cu in this alloy, it will also be significantly prone to the formation of S_Al2CuMg. The 7075 alloy has a lower Zn:Mg ratio of 2.2 and although still predominantly hardened by rj, some T phase Table 10.1 Composition and Zn/Mg ratio of various 7XXX alloys (after Polmear 1989). Values for Si, Fe and Mn relate to maximum values Alloy Si Fe Cu Mn Mg Zn Cr Zn/Mg AA7049 0.25 0.35 1.5 0.2 2.5 7.7 0.15 3.1 AA7050 0.12 0.15 2.3 0,1 2.3 6.2 0.04 2.7 AA7075 0.4 0.5 1.6 0.3 2.5 5.6 0.23 2.2 AA7079 0.3 0.4 0.6 0.2 3.3 4.3 0.18 1.3 References are listed on pp. 402-408. (a) til v) < a: a. a o s X c a j o s 100 200 300 400 500 600 700 TEMPERATURE CELSIUS 100 200 TEMPERATURE CELSIUS Figure 10.51 Calculated mole % phase vs temperature plots for 7XXX series Al-alloys. (a) AA7049, (b) AA7050, (c) AA707S and (d) AA7079. AA7049 (Al) f Liq \ \ \ '■ -: ^illl 1 \ - ~ ^ i . \ 1 *r i : \ I >^ t 'r . -4., TIs^^ References are listed on pp. 402-408. uj < X -i o 3 100 200 300 400 500 600 700 TEMPERATURE_CELSIUS ( — O < o 950 900 850 800 - 750 700 " 650 " 600 U720 U720LI Figure 10.59 Variation in calculated tr-solvus temperature as elements in U720LI change between maximum and minimum specified limits. References are listed on pp. 402-408. 360 N. Saunders and A. P. Miodownik 10.6.3.3 Liquid-phase sintering of high-speed M2 steels. High-speed steels, which typically contain at least seven elements, can be produced in a variety of ways, for example by casting, by water or gas atomisation with subsequent hot compaction of the atomised powder, and by liquid-phase sintering. The latter provides a production route whereby the steel can be produced directly to the correct shape. The process relies on there being sufficient liquid to infiltrate the pores of a powder compact and produce densification, but not too much, as this would cause the compact to lose structural strength and distort. A reasonable level for liquid-phase sintering is approximately 10% of the volume. It is also critical that the volume of liquid is fairly insensitive to fluctuations in temperature in the furnace, i.e., dViiq/dT is as small as possible, otherwise the sensitivity of the process to fluctuations in temperature control, or the intrinsic variations in temperature within the furnace itself, makes the process uncontrollable. Figure 10.60 shows a phase % vs temperature plot for an M2 steel with a composition (in wt%) of Fe-6.2W-5.lMo-4.2Cr-l.85V-0.3Si-0.8C. The alloy is characterised by the formation of two types of carbide, M6C, which is the predominant form, and MC. The calculated melting temperature is close to that observed for such alloys and the amount of M6C and MC is also in good agreement with experimental observation (Hoyle 1988). Chandrasekaran and Miodownik (1989,1990) and Miodownik (1989) examined M2 steels, with particular emphasis on the effect of increasing V levels to increase the formation of the V-rich MC carbide. Figure 10.61 shows the change in behaviour of M2 when the V level is increased from 1.85 to 2.5wt%, calculated using Fe-DATA (Saunders and Sundman 1996). The MC carbide is stabilised as expected, but a is also stabilised and becomes involved in a fairly complex reaction scheme with the liquid, 7, M6C and MC. Both of these effects are qualitatively expected, but now the CALPHAD route enables calculations to be made for the amount of liquid as a function of temperature. Figure 10.62 shows such calculations as V levels are raised from 1.75% to 2,5% and the increase in solidus temperature with increasing V addition reflects well the experimental measurements quoted by Chandrasekaran and Miodownik (1989). It can now be seen that the slope of the liquid curve is flat for the lower levels of V, i.e., dVíiq/dT is small, but as the V levels reach 2.5wt%V, the slope becomes steep. Clearly there will be a limit around this composition at which the alloy will become difficult to fabricate by liquid-phase sintering. 10.6.4 Intermetallic alloys Intermetallic alloys (compounds) are becoming of increasing interest as materials which possess significantly enhanced high temperature capabilities compared to many conventional metallic alloys. However, they suffer intrinsic problems associated with low-temperature ductility and fracture toughness. Two types of CALPHAD—A Comprehensive Guide 361 References are listed on pp. 402-408, < S a O S 1400 1500 MC TEMPERATURE CELSIUS Figure 10.60 Calculated mole % phase vs temperature plot for an M2 steel with normal V level. w < as w J o 1100 1 1200 MC 1300 1400 TEMPERATURE CELSIUS 1500 Figure 10.61 Calculated mole % phase vs temperature plot for an M2 steel with high V level. iv. oaunaers ana a. r. mivuvwmn, 20 15 16 O 12 tS 10 o — /1 ' — /! < ; - / / •'' / / - / //7 /// '/ Low V ; ,f \ - ^7 / ^High V i/ /; / 1 1 1240 12S0 1260 1270 1280 1290 TEMPERATURE_CELSIUS Figure 10.62 Calculate mole % liquid vs temperature plots for an M2 steel as V levels are changed between 1.75 and 2.5wt%. intermetallic alloys have attracted wide attention, those based on NiAl and those on TiAl. The next two sections describe work on both types of alloy. 19,6.4.1 NiAl-based intermetallic alloys. Phase-diagram studies have been used extensively in NiAl-based alloys as a method of designing microstructures. NiAl is difficult to prepare as a binary alloy with reasonable levels of ductility and fracture toughness. Therefore considerable effort has been placed in designing micro-structures which might reduce this inherent brittleness. An approach has been to make alloy additions to NiAl so that it forms a two-phase structure with a more ductile phase, such as the f.c.c. Ni-Fe-based solid solution, 7, (Ishida et al. 1991), or even 7' based on Ni3Al (Kainuma et al. 1996). This has been shown to produce high levels of ductility for such materials but, unfortunately, the process of ductilisation by a softer second phase does lead to a degradation of intrinsic strength and high-temperature creep capability. Another approach to designing NiAl alloys has been to produce multi-phase structures containing NiAl + other intermetallic compounds such as the Heusler-type phase Ni2AlTi and 7' (Yang et al. 1992a,b). These alloys are less ductile but have significantly higher yield strengths and potentially enhanced creep properties. The approach of Ishida et al. (1991) and Kainuma et ah (1996) utilised both experimentally determined and calculated diagrams for Ni-Al-Fe (Fig. 10.63) to References are listed on pp. 402-408. IF*" (a) Isothermal Section at T=1100°C 60, 20 40 at% Al 60 (b) Ni-25Al-XFe Vertical Section 1 Figure 10.63 Phase equilibria in the Ni-Al-Fe system from Kainuma et al. (1996). define compositions whereby various mixtures of NiAl and 7/7' could be produced. These authors optimised their alloys on the basis of the amounts of the various phases as well as their microstructure. In their case, the initial microstructure was an Ll0 martensite formed by transformation of the /? phase on cooling. By using a series of heat treatments and varying the composition of the alloy they were able to design three distinct types of microstructure (Fig. 10.64) and successfully produce \ T<200TC Llo Martensite B2 /? + y '(widman.) up -^ T>2O0t: —> «\\™ .yain.-tj'pe IlVvJsS ■iiiHl Llo Martensite NisAb @ + y "(lam.-type 11) jS+y'Cblocky) Room Temp. 30ot; 7oot: soot; Heating Temperature Figure 10.64 Schematic illustrations showing the microstructural evolution of three kinds of 0 + 7' microstructures; widmanstatten, type 1 lamellar and blocky type 2 lamellar structures in Ni-25Al-{a)18Fe, (b)15Fe and (c)13Fe alloys. NiAl-based alloys with ductilities as high as 10% in tension and strengths in the region of 750-1000 MPa. Yang et al. (1992a, b) also utilised a combination of experiment and calculation to critically determine the phase region for the /3-NiAl, 7'-Ni3Al and /?'-Ni2AiTi phases. The philosophy of their approach was to produce an alloy with high levels of /? and /3', as mixtures of these phases had been shown to have enhanced creep resistance in comparison to the monolithic phases themselves (Polvani et al. 1976). The combination of experiment and calculated phase % vs temperature plots (Figs. 1600 600 800 1000 1200 1400 1600 Temperature, °C Figure 10.65 Calculated mole % phase vs temperature plots for Ni-AI-Ti intermetallic alloys, (a) Ni-28Al-12Ti, (b) Ni-22Al-15Ti and (c) Ni~20Al-!3Ti. 10.65(a-c)) allowed precise microstructures to be denned and subsequently produced in candidate alloys. In these alloys the microstructure was as much controlled by the solidification mechanism as by any solid state transformation and, as such, the calculations were invaluable as they could be used to predict solidification patterns. Alloys produced as part of this programme had high compressive yield stresses, in the range of 1000-2000 MPa, and, although the alloys still had quite low tensile ductility, there is a significant enhancement in ductility due to the generation of dislocations at interphase boundaries. References are listed on pp. 402-408. 366 N. Saunders and A. Jf. Mioaowmk 10.6.4.2 TiAl-based intermetallic alloys. Alloys based on the 7-TiAl compound are still very much in the early stages of development. Commonly used variants such as Ti-48Al-2Mn-2Cr and Ti-48Al-2Mn-Nb (at%) are quaternary in nature and it is only recently that alloys of a multi-component nature have been developed. As alloy development has progressed, increasingly complex behaviour has been observed and changes in transformation behaviour can now be tracked using a recently developed TiAl database (Saunders 1997b). All alloys are based on the 7-TiAl compound of Ti-Al and Fig. 10.66 shows the calculated diagram for the binary system Ti-Al. Alloys usually contain between 43-50at%Al and, forth© most part, contain a2-Ti3Al as well as 7-TiAl. They are usually heat treated in the high-temperature, single-phase a-phase region, or just below it, before cooling when the a phase decomposes to a microstructure which exhibits a fine lamellar structure of transformed 7-TiAl with fine laths of a2-Ti3Al. Figure 10.67 shows a mole% phase vs temperature plot for a Ti-48A3-2Mn-2Nb alloy of nominal composition; variations of this alloy with Al in the range 45-48at% are commonly used. It is a straightforward 02/7 alloy which can be heat treated in the a condition before transforming on cooling to (02 + 7) and very much exhibits the prototype microstructure for the early type of alloys. The replacement of Mn by Cr in the Ti-48Al-2Cr-2Nb alloy (Fig. 10.68) causes the predicted onset of instability with respect to a Cr-rich B2 phase. This in good accord with experimental observations in alloys of this type (Fuchs 1995, Kelly and Austin 1996) and at low temperatures there is also a potential for the formation of 1800 1600 c/5 2 1400 a o < w a 1200 1000 - 800 600 400 - Liq p AlnTi5 _ /y a 1 Y I Al3Ti \ / «2 1 / 1 1 1 I 1 1 20 40 60 Al,Ti 80 100 MOLE_PERCENT AL Figure 10.66 Calculated Ti-Al phase diagram. (Al) References are listed on pp. 402-408. 600 800 1000 1200 1400 TEMPERATURE CELSIUS 1600 Figure 10.67 Calculated mole % phase vs temperature plot for a Ti~48Al~2Mn-2Nb alloy. w ■Si < 33 CL, U5 -J O 5 a-Cr 600 800 B2 1000 1200 1400 TEMPERATURE CELSIUS 1600 Figure 10.68 Calculated mole % phase vs temperature plot for a Ti-48Al-2Cr-2Nb alloy. :50B iv. duunutsrs uriu si. 4 . iviiuuuwiur\ Table 10.2. Some recent 7-TiAl-based alloys with comparison between experimentally observed and calculated a-transus temperatures a-rransus a-transus Alloy (exp.) (calc.) Reference Ti-48Al-2Cr-2Nb 1364 1357 Fuchs (1993) Ti-49.5A1-1.1 Mn-2.5Nb 1436 1425 Lombard et at. (1992) Ti-47Al-2.SNb-lCr-lV 1350 1357 Kim (1992) Ti-46.7Al-3Nb-lW 1350 1353 Bhowa! et al. (1995) Ti-48Al-2Nb-2Cr-lW 1358 1371 Fuchs(1995) Ti-47A1-1.5Cr-O.5Mn-2.6Nb-0.15B 1365 1367 Kim (1995) Ti_47Al-2Nb-lMn-0.5W-0.5Mc-0.2Si — 1366 Seo et al. (1995) almost pure Cr. Newer alloys have centred around the substitution and addition of elements to the 48-2-2-type alloys and have compositions of the type shown in Table 10.2, which also gives comparisons for experimentally observed and calculated a-transus temperatures. It is noticeable that heavy elements such as W and Ta are now being increasingly used and that alloys are subsequently becoming more prone to formation of the B2 phase. This is seen for example in alloys such as Ti-48Al-2Nb-2Cr-lW, and their variants (Fuchs 1995). One of the most complex alloys developed so far is Ti-47Al-2Nb-lMn-0.5W"0.5Mo-0.2Si. However, although truly multi-component in nature, the total refractory metal addition to a basic Ti-Al alloy is still only 4at%. The microstructure of this alloy consists of second-phase particles enriched in Mo and W and there is also evidence for silicides (Seo et al. 1995). Figure 10.69 shows the calculated phase % vs temperature plot for this alloy; the alloy is predicted to be unstable with respect to a B2 phase enriched in Mo and W, and Ti5Si3 will form below 1020°C. The calculation also predicts that the alloy may become unstable with respect to W precipitation at low temperatures. It is clear that as these alloys have become more highly alloyed, the simple prototype concept of an 012/7 microstructure is having to be modified to take into account borides, silicides and the B2 phase. It is now possible to understand the role of the various elements in promoting these phases and also to design with them in mind. For example, the B2 phase can inhibit grain growth if it is present in the high-temperature a-phase field. This appears somewhat analogous to conventional Ti alloys, where some small amounts of a in /? grain boundaries during processing and help prevent catastrophic grain growth during forging, but the role of the phases is completely reversed. 10.6.5 Alloy design Most of the previous examples show that CALPHAD calculations can enhance knowledge of the general phase behaviour of alloys when a suitable thermodynamic References are listed on pp. 402-408. < X a _) O S -Liq 600 / 800 a-W TEMPERATURE CELSIUS 1000 TisSi3 1400 1600 Figure 10.69 Calculated mole % phase vs temperature plot for a Ti-47Al-2Nb-lMn-0.5W-0.5Mo-0.2Si alloy. database is available. However, it is also interesting to look at some CALPHAD-based work where the main aim has been to help design or optimise some specific feature, or combinations of features, which are affected by phase behaviour. Such features may be associated with a physical property such as modulus and magnetism, a mechanical property such as strength, a chemical property such as corrosion resistance or some more complex combination which might effect a property such as weldability. The best examples centre around Fe-based materials, which probably relates to historical reasons as Fe-based systems were one of the first types of alloy to be thermodynamically characterised in any great detail. However, it is clear that once good thermodynamic characterisations are available the use of CALPHAD methods need not be limited to any particular material type (Miodownik 1993). 10.6.5.1 Magnetic materials. The value of CALPHAD calculations for magnetic alloys has been demonstrated for Fe-Cr-Co-based alloys, where alloys with improved magnetic properties were made by designing their composition and heat-treatment temperature to lie in a miscibility caused by magnetic forces (Nishizawa et al. 1979a, Homma et al. 1981, Ishida and Nishizawa 1991), Inden (1987) has described in detail the background to the production of such hard magnets which can be summarised as follows. A good design for a hard magnetic material is to have small, elongated particles, 5 IV aligned and magnetised along their axis, embedded in a paramagnetic matrix. One of the easiest ways to produce such a microstructure is by some form of precipitation reaction, where the size of the particles can be controlled by heat treatment. This then leaves the problem of producing the requisite shape and alignment of the particles which leads to a further prerequisite that the precipitate/matrix interface must have a low energy. It is not always possible to produce 'ideal' rod shapes, but precipitates with a more plate-like morphology can also be aligned by applying a magnetic field during the precipitation process. For such materials it is desirable for there to be a miscibility gap due to magnetism (Fig. 10.70(a,b)) as described in Chapter 8. In these circumstances, spinodal decomposition can occur by the formation of paramagnetic and ferromagnetic phases. The best magnetic properties can be produced if annealing is performed just below the temperature where instability begins. Figure 10.71 shows a calculated isothermal section for Fe-Cr-Co at 1200 K, showing how the miscibility gap in the binary systems is expanded in the ternary. It should be noted that these sections are metastable, as the a phase would precipitate out in equilibrium. However, if heat treatments are done for sufficiently short times, spinodal decomposition occurs without precipitation of a. The effect of the expansion of the miscibility gap in the ternary means that higher heat-treatment temperatures can be used, allowing a material with a higher Curie temperature and subsequently higher saturation magnetisation to be produced. Heat treatments for these alloys can be sensitive to small changes in composition. Figure 10.72 shows a vertical section in Fe-Co-Cr at a ratio of x$e/zco = 83/17 and it can be seen that only a few at% differentiates alloys with a paramagnetic or a ferromagnetic matrix. Al-Ni and Al-Ni-Co magnets work on identical principles to the Fe-Cr-Co magnets but, instead of considering a miscibility gap between paramagnetic and ferromagnetic phases which are disordered, the paramagnetic phase is, in this case, ordered. Figures 10.73(a,b) show an isothermal and a vertical section through the Fe-Ni-Al ternary system produced by a combination of experiment and calculation (Hao et al. 1984). Additions of Co were made to this basic system and, in accord with thermodynamic calculations (Nishizawa et al. 1983), both the peak temperature of the miscibility gap and the region of immiscibility in the quaternary are increased. Good magnetic properties in these alloys are obtained under the following conditions: (1) The ferromagnetic c*i phase is present as isolated particles embedded in a weakly magnetic or non-magnetic matrix of az\ (2) the particles are uniaxially aligned; and (3) the volume fraction of a.\ is in the range 0.4-0.6 Unfortunately, Al-Ni and Al-Ni-Co magnets suffer from the disadvantage of being hard and brittle, leading to problems with machining which becomes expensive and difficult. Using a mainly experimental phase-diagram approach, Ishida et al. (1991) were able to design an alloy which contained a small amount of ductile fee. 7 phase distributed along the grain boundaries of the alloy. This References are listed on pp. 402-408. - i 1 "i I 1200 1000 0 A 0.2 0.4 0.6 0.8 1.0 MOLE FRACTION B 0.5 Figure 10.70 (a) Phase diagram for an A-B alloy system exhibiting phase separation due to magnetism and (b) underlying Gibbs energy vs composition curve showing the contribution from chemical and magnetic energies (from [nden 1987). Figure 10.71 Calculated isothermal sections for Fe-Cr-Co at 1200 K (from Inden 1987, Nishizawa et al. 1979b). 372 JV. oaunaers unu .1. 1 . imuu B matrix ct„ Figure 10.72 Calculated vertical section through the Fe-Cr-Co system at a constant ratio xFe:xCo of 83:17 (from Inden 1987, Homma et al. 1981). Te is the Curie temperature. microstructure significantly improves hot workability and leads to the possibility of producing ductile material. 10.6.5.2 Rapidly solidified in-situ metal matrix composites. A design project for alloys based on the Fe-Cr-Mo-Ni-B system, and produced by rapid solidification, was undertaken by Pan (1992). During processing a mixture of borides is formed inside a ductile Fe-based matrix which makes the alloys extremely hard with high moduli. These alloys provide a good example of how phase-diagram calculations were able to provide predictions which firstly helped to identify unexpected boride formation (Saunders et al. 1992) and were ultimately used in the optimisation of the modulus of a shaft material for gas turbines (Pan 1992). The alloys are first produced by rapid solidification and are amorphous in nature. They are either directly fabricated as powders, by a process such as high-pressure gas atomisation (HPGA), or by melt-spinning of ribbons, which are subsequently pulverised to form a powder (<150 /an). The powders are then consolidated by hot extrusion between 950-1050°C where the initial amorphous structure breaks down and forms a fine dispersion of stable borides in a ductile Fe-based matrix. 97.5 Fe + 2.5S SO o Concentration of Fe/at% Y/ Niai \\.25%a\ Figure 10.73 (a) Isothermal and (b) vertical sections from the Ni-Fe-Al phase diagram (Ishida and Nishizawa 1991). References are listed on pp. 402-408. Because of the inherently non-equilibrium nature of the production route, the first question which needed to be answered was whether the phases present in the alloy were in fact stable, so that equilibrium calculations could actually be used to design these alloys. To this end CALPHAD calculations were combined with a detailed experimental characterisation of a Fe7oCri8Mo2Bio alloy (Kim et al. 1990, Pan 1992). The TEM and XRD results confirmed earlier work (Xu et al. 1985) which stated that an orthorhombic boride M2B was present and its composition was Cr-rich. However, they also showed that a proportion of the borides (~10%) were Mo-rich and that the Fe-based matrix was martensitic. The latter result was particularly surprising because of the high level (20at%) of a-ferrite stabilisers Cr and Mo. Furthermore, initial analysis of diffraction patterns from the TEM work indicated that the structure of the Mo-rich boride was a tetragonal type whose structure had not been reported in previous literature (Kim and Cantor 1988). Calculated phase equilibria for this alloy produced the following predictions: (1) The existence of a Cr-rich M2B phase. (2) There would be a substantia] proportion (7.3%) of the U3Si2-tvpe, M3B2 boride in the alloy with high levels of Mo. (3) The Fe-based matrix would be austenitic at 1000°C but transform to ferrite below 857°C, thus giving a reason for the observed martensitic structure. Based on the prediction for the M3B2 boride, and its observed lattice parameter variation with Fe, Cr and Mo levels, the structure of the Mo-rich phase was reevaluated and clearly shown to be primitive tetragonal of the U3Si2-type (Kim et al. 1990). This work also gave results for ratio of Fe:Cr:Mo in the various phases which were in excellent agreement with those predicted at 1000°C. It is clear that the input of the phase-diagram predictions greatly helped in understanding the evolution of microstructure in this alloy, and although the alloys were produced by a highly non-equilibrium route, the calculations also showed that the phases present after extrusion were the stable phases for the alloy, so design criteria based on equilibrium calculations could therefore be used. A further advantage of the calculation route was that the number of alloys which needed to be examined, in order to achieve the optimum microstructure/properry combination for the design criteria of the turbine shaft, could be dramatically reduced (Pan 1992, Miodownik 1993). In order to evaluate the role of the various phases, it was necessary to design distinct alloys where the matrix was either austenitic or ferritic. Figure 10.74 shows the principle by which this was achieved for Fe-Cr-B alloys where it can be seen that only a small change in Cr level puts an alloy into a region where it is fully ferritic at consolidation temperatures. Alloys from the Fe-Cr-Mo-B system were then designed so that the matrix was fully ferritic and a further set of alloys from the Fe-Cr-Ni-B system which were fully austenitic. Although producing stable microstructures, significant drops in strength and hardness were found in alloys 0.1 0.2 0.3 a 0.4 0.5 MOLE-FRACTION CR Figure 10.74 Calculated isothermal for Fe-Cr-B at 1000°C showing placement of high-B alloys which have either a or 7 matrices at processing temperature (Pan 1992). oh O ~3 T3 o s c 600 500 400 300 200 100 0 -Eshelby Model ■ Modified 31 Heat Treated 0 0.2 0.4 0.6 0.8 1.0 Volume Fraction of Boride Figure 10.75 Comparison of calculated Eshelby curves for modulus with experimentally determined moduli for high-B ferrous base alloys (Pan 1992), whose matrix was either fully ferritic or austenitic. It also became clear that small amounts of C were present in all alloys which was adding to the hardness of the martensite, hence enhancing its properties. The next step was to optimise the ratio of M3B2 to MB2 and various alloys were designed and tested to improve factors such as strength and modulus (Pan 1992). Eshelby analysis (Eshelby 1957, Withers et al. 1989) was used to predict modulus and good agreement was found with experimental measurement (Figure 10.75). It References are listed on pp. 402-408. was clear that modulus was significantly enhanced by increasing boride level but owing to morphological considerations (the borides were not aligned and had low aspect ratios) the modulus increase was less than was hoped for. In the end, alloys were designed to have martensitic matrices, approximately equal volumes of M3B2 and MB2 and predicted modulii of between 245-255 GPa. All of these properties were achieved in the final experiments . One of the limiting factors in looking at higher amounts of M3B2, which were more finely dispersed and, hence, potentially gave greater strength, was that high liquidus temperatures made it difficult to melt such alloys. 10.6.5.3 The design of duplex stainless steels. Lee (1995) reported on work relating to the design of duplex stainless steels using a predominantly thermodynamic approach. Four important properties were chosen as being critical to performance, and these were: (1) strength, (2) toughness, (3) weldability and (4) corrosion resistance. Of these, strength was considered to be the least critical in the alloy design process, as this was heavily controlled by factors such as work hardening and grain size, and would be more effectively controlled by thermo-mechanical processing rather than design of composition. Lee (1995) then identified critical factors associated with phase equilibria which would affect the other three properties. These were the stability of austenite at high temperatures for weldability, sigma formation for toughness and the composition of austenite in local equilibrium with M23C6 for corrosion resistance. These factors could then be combined to give an overall performance criterion. The rationale for the choice of favourable thermodynamic properties was based on the following arguments. Weldability. It had been previously reported (Norstrom et al. 1981) that an increase in austenite amount was beneficial to weldability. Further, Cao and Hertzman (1991) had reported that loss of impact toughness because of ferrite formation during welding could be recovered by re-formation of austenite at lower temperatures. Lee (1995) subsequently concluded that increased stability of austenite above the heat-treatment temperature would be beneficial to weldability. Therefore, the amount of austenite at 1350°C was taken as a criterion for alloy design, higher values being given a positive rating compared to lower values. Sigma formation. While o--phase formation is known to cause embrittlement in duplex stainless steels, Lee (1995) argued that the important factor in the process was the driving force for precipitation rather than the potential amount of a which might be formed. This was because only small amounts are actually necessary to cause embrittlement (Norstrom et al. 1981) and, therefore, the early stage of precipitation should be considered more important than the final equilibrium state. While nucleation is a complex process, Lee (1995) suggested that, for the purpose of alloy design, nucleation parameters for a such as interfacial energies, misfit strain energies, etc., would be approximately equal for alloys which lay close in composition to the original alloy. This would mean that the driving force for Table 103. Composition of candidate alloys and results of calculations on toughness, weldability and corrosion resistance. Calculation was conducted assuming an annealing temperature of 1050°C O.S%Mn, 0.7%Si and 0.024%C Cr>W. As carbides other than M2C would also form in their alloys, they plotted driving forces to form M23C6 and M6C, which are shown in Figs. 10.76(b, c). It can be seen that the lowest driving forces to form these carbides were in Mo-rich alloys and, hence, such alloys would maximise the yield of M2C. Grujicic (1991) then made a series of calculations to estimate the M2C coarsening rate in these types of alloys. This is important because metastable cementite is often a predecessor precipitate to M2C and deleterious to mechanical properties. The cementite can be removed by prolonging the tempering treatment, but this causes subsequent coarsening of the desirable M2C. Using simple coarsening theory, they were able to determine that W-rich alloys would have the greatest resistance to Cr (2.17 wi' Fe-HCo-10Ni-0.25C-(W-Mo-Cr) T = 783 K Fe-14Co-10Ni-0.25C-(W-Mo-Cr) T = 783 K. Fe-14Co-10Ni-0.25C-(W-Mo-Cr) T = 783 K. Figure 10.76 Variation of the driving force (kJ mol"1) for precipitation of (a) M2C, (b) M23C6 and (c) M6C from ferrite at 783 K in a Fe-14Co-10Ni-0.25C-(W-Mo-Cr) alloys with balanced alloy additions of Mo, Cr and W {Grujicic et al. 1987). References are listed on pp. 402-408. 380 N. Saunders and A. P. Miodownik Cr (2.17 w/o) Fe-14Co-10Ni-0.25C Coarsening rate of M2C T = 783 °K IE-19 W (7.65 w/o) Mo (4.0 w/o) Figure 10.77 Coarsening rate of M2C at 783 K in a Fe-l4Co-I0Ni-0.25C- 1/3 (CA (1-2JCJ8Q,) {xA„oMAn0 + xSiO,MSi0l) _%Si02_ (xAnoMAno + afciOjMsioJ /I -a:siO?Y \ 2a;Sio2 / (10.5) (10.6) References are listed on pp. 402-408. 384 and N. Saunders and A, P. Miodownilc C% = 1000 MSKA 1a„$ (10.7) where x and M denote, respectively, the moles and molecular weights of the various components. The Henrian activity coefficient of AnS, 7^ s, is then assumed to be equal to 1, and if Ka for each component is known, the sulphide capacity can be calculated for each oxide component. Values of Ka were obtained from assessed thermodynamic values. The various values of Cs for each oxide component were then obtained from the following equation: log CS = va log Cs{a) + vb log Cs(b) + vc log Cs{c) + ■ (10*8) where log CA{S) >s me value of log Cs in the binary AnO-Si02 at the same value of xsi02 as in the multi-component system and va = xano (10.9) The approach yielded excellent results and Figs 10.80-10.83 show comparison of calculated and experimentally determined sulphide capacities in various multi-component slags. -3.2 -3.4 I503°C O FeO • MgO FeO -4.2 MgO 8 12 16 Wt. % FeO, MgO or A1203 20 Figure 10.80 Comparison between calculated and experimental (Bronson and St-Pierre 1981) effects of A1203, FeO and MgO additions upon sulphide capacities of CaO-Si02 slags at a constant (CaO+AO)/(Si02+Al203) ratio, where A=Fe or Mg. \sAL.rnj\ij—a uomprenensive uujuc 0.2 0.4 0.6 0.8 1.0 XMnc/ (XMnO+XMgo) Figure 10.81 Comparison between calculated and experimental {Sharma and Richardson 1965) sulphide capacities at constant Si02 fraction in MnO-MgO-S>02 slags. 1650°C 160CC 1575°C -1 -3 o a -J r~ 0 i~ 1 - -2 — 0 - -1 - -3 - -2 - -4 - -3 -5 L -4 1650°C -— • __^—"""^• 1600°C □ 1575°C I 1 1 0 Calculated • Experimental 1 1 0.0 0.1 0.2 0.3 0.4 0.5 XCaO+0-1XMgO-0-8XA!2O3_XSiO2 Figure 10.82 Comparison between calculated and experimental (Bronson and St-Pierre 1981) sulphide capacities in Si02-Al203-MgO-CaO-FeO slags. References are listed on pp. 402-408. 386 N. Saunders and A. P. Miodownik CALPHAD—A Comprehensive Guide 387 0.0 0.1 0.2 0.3 0.4 XA1203 Figure 10.83 Comparison between calculated and experimental (Fincham and Richardson 1954, 1964, Sharma and Richardson 1965) sulphide capacities in AO-Si02-Al203 slags (where A = Mn, Mg, Ca) at a constant Si02 fraction of 0.4. 10.6.6.3 Estimation of liquidus and solidus temperatures of oxide inclusions in steels. The deformation of inclusions in steels has significant consequences on the hot workability of steels as well as for the mechanical properties of the final product. In order to increase their deformability there are at least three strategies (Matsumiya et ah 1987): (1), Reduction of their melting point; (2), deceleration of crystallisation; and (3), reducing their flow stress. If the melting point can be reduced sufficiently so that some liquid is present at the hot-working temperature, the inclusions would be expected to deform easily. To this end, Matsumiya et al. (1987) made calculations for inclusions from the quinary system Si02-Al203-CaO-MgO-MnO, based on assessments of the component binary and ternary sub-systems. Figures 10.84(a,b) show two of the calculated ternary diagrams and Table 10.4 shows comparisons between calculated and experimentally determined liquidus temperatures for five oxide inclusions. Figures 10.85(a, b) show phase fraction plots for inclusions 1 and 2 in Table 10.4. These are plotted in such a way as to show the cumulative amount of all phases as well as their individual amounts. A quasi-ternary diagram was then plotted for an 'ideal' inclusion with a fixed level of Al2O3=20.4wt% and MgO=8.2wt% (Fig. 10.86). From this it can be seen that a slight increase in Si02 reduces the liquidus CaO 20 40 60 80 FeO wt% FeO Si02 CaO 20 40 60 80 MgO wt% MgO Figure 10.84 Calculated isothermal sections at 1600°C for (a) Ca0-FeO-SiO2 and (b) CaO-MgO-SiOj (Matsumiya et al. 1987). temperature of inclusion 1 from Table 10.4. Taking this into account in a new 'ideal' inclusion, they made further calculations by varying the various levels of the component oxides with fixed SÍO2 content. From these calculations they were able to conclude that the liquidus temperature was sensitive to changes in the component oxides with sensitivity factors in the following order: MnO>Al203>MgO>CaO. To realise the potential reductions in liquidus temperature of the inclusions, changes would be needed during the steelmaking process in the de-oxidiser, refining slags and refractory materials. References are listed on pp. 402-408. Table 10.4. Compositions, Eiquidus temperatures and primary phases of oxide inclusions Oxide composition (weight fractions) Liquidus (°C) No. Si02 AI2O3 CaO MgO MnO Calc. Exp. 1 0.459 0.204 0.153 0.082 0.102 1290 1300 2 0.500 0.050 0.020 0.230 0.200 1390 1404 3 0.4208 0.2956 0.2108 0.0441 0.0287 1450 1460 4 0.5081 0.3559 0.0833 0.0437 0.0090 1550 >1500 5 0.7749 0.1830 0.0012 0.0054 0.0355 1280 >1650 6 0.5647 0.2712 0.0270 0.0010 0.1361 1470 >1500 Primary phase MgO.A!203 2MgO.Si02 Ca0.2Si02.Al203 Ca0.2Si02.3Al203 2SÍ02.3A1203 2Si02.3Al20j a) w < X a. u. O * z o p < M Pl, W J O S 1.0 (a) 0.5 0.0 sío2 ^Ts= 1080°C ~"""jMnO-AI,03 Liquid - *" /^Mg0-SiO2 Yj.Ca0'SiO2 ^\-CaO-MgO CaO-2S i 02-AI203 _^^/^\^MgO-AI20, JP\ T, = 1290°C >--1 - s* 1000 1100 1200 1300 1400 TEMPERATURE °C 1500 (b) 2MgO-Si02 1100 1200 1300 1400 TEMPERATURE'C 1500 Figure 10.85 Calculated phase fraction vs temperature plots for oxide inclusions nos (a) 1, (b) 2 and (c) 3 from Table 10.4. SiO. MgO-SiO, 20.4wt% WMgO = 8-2wt% CaO'2SiO Al,0 2OV0 (0 : composition No. 1) CaO MgO-At203 MnO Figure 10.86 Calculated liquidus surface of the five-component oxide system with fixed values of 20.4wt%Al2O3 and 8.2 wt%MgO. 10.6.7 Complex chemical equilibria 10.6.7.1 CVDprocessing. CVD (chemical vapour deposition) processing is an area where calculations using mainly a substance database have proved valuable in understanding the process conditions for deposition of silicides, borides, carbides, etc. A good example of such calculations is provided by Vahlas et al. (1996) who looked at the deposition of WSi2 from various gaseous environments. They utilised a substance database for the elements Si-W-Cl-H-O-Ar where 46 species in the gas phase and 20 stoichiometric condensed phases were considered in the calculation. They first calculated a so-called 'CVD diagram' for the system WF^-SirLr-Fir-Ar, representing the incoming gas, which shows the phases which will be deposited as a function of partial pressure of WF6 and SiH4 (Fig. 10.87). The lines separating the various deposition regimes have 'bands of uncertainty' superimposed to reflect the uncertainty arising from the assessment of the thermodynamic data for the total system. It is clearly seen that the deposition ofpure WSi2 will be difficult using these input gases. In order to find a less sensitive system the case of WCU-SiHr-H/r-Ar was considered, whose CVD diagram is shown in Fig. 10.88. It can now be seen that the single-phase region for WSi2 has significantly expanded which means that the CVD process will be less sensitive to composition fluctuations in the input gas References are listed on pp. 402^108. 390 JV. Saunders and A. P. Miodownik CALPHAD—A Comprehensive Guide 391 itself, or fluctuations in the gas due to transport phenomena within the CVD deposition chamber. Further variations occur when SiH4 is substituted for by SiCl2H2 and the width of the WSi2 single-phase region expands even further (Fig. 10.89), providing even less demanding conditions for the deposition of pure WSi2. PSiH4 Figure 10.87 Calculated CVD phase diagram for the WFs-SilVH^Ar system at 7> 1000 K, Pkoi = 1 atm and ^=0.9 atm (from Vahlas et al. 1996). PsiH4(aim) Figure 10.88 Calculated CVD phase diagram for the WCl2-SiH4-H2-Ar system at T= 1000 K, Pw\= 1 atm and ^=0.9 atm (from Vahlas et al. 1996). The substitution of TiCl4 for WCL, yields the CVD diagram as shown in Fig. 10.90 (Vahlas et al 1996) and it can clearly be seen that the CVD diagram is totally different, demonstrating both the system specific nature of such diagrams and the importance of the underlying thermodynamics in determining how the process will occur in practice. Figure 10.89 Calculated CVD phase diagram for the WCl4-SiCl2H2-H2-Ar system at T= 1000 K, 1 atm and Pu = 6.9 atm (from Vahlas et al. 1996). Figure 10.90 Calculated CVD phase diagram for the TiCL,-SiRt-H2-Ar system at T= 1000 K, /"toul= 1 arm and ^„=0.9 atm (from Vahlas et al. 1996). References are listed on pp. 402-408. 392 N. Saunders and A. P. Miodownik K^ALftiAu—a isomprenensive uw<«e 10,6.7.2 Hot-salt corrosion in gas turbines. In a wide variety of cases, Ni-based super-alloys are protected from corrosive attack in gas turbine engines by the formation of a surface layer of Cr203. However, in marine environments, NaCl can become concentrated in the incoming gas and lead to reaction with sulphur-containing combustion products to form Na2S04. This then condenses onto the Cr203 layer which leads to the dissolution of Cr203, exposing the alloy itself to corrosive attack from the atmosphere, which is both oxidising and sulphidising. This type of attack is often called 'hot-salt corrosion' and Barry and Dinsdale (1996) examined this process using a substance database as the basis for their calculations. The required data is for the gas and solid phases in the system NaCl-NaOH-Na2Cr04-Na2S04. Some solubility was allowed for in the condensed solid phases, mainly in terms of binary interactions between the respective components which form simple phase diagrams (see for example Fig. 10.91). Calculations were then made relating to a gas turbine operating at a fuel/air ratio of 50:1, at 15 bar and 750°C. The fuel was taken to have a composition approximating to the formula CHi.8. On the basis of these assumptions, the combustion products were calculated to be predominantly N2, 02, C02 and H20, their respective partial pressures being, 11.6,2.216, 0.61 and 0.55 bars. 1% sulphur in the fuel would then cause the sum of the pressures of S02 and S03 to be 0.0026 bar. If only 1 ppm of NaCl were present this would cause the partial pressure of HC1 in the gas to be 0.0046 bar, the residual sodium forming mainly as Na2S04 on any exposed surfaces. 1200 iioo 1000 wo s u 800 600 500 Liquid Hexagonal Figure 10.91 Calculated phase diagram for the ^SCVNajCrO, binary system (Barry and Dinsdale 1996). 10.6.7.3 Production of silicon in an electric arc furnace. Although not particularly complex in terms of chemical equilibrium, the production of Si in an electric arc furnace is a neat example of how equilibrium calculations can be made which take into account material flow during a dynamic process (Eriksson and Hack 1990). In practice, the furnace works continuously, with raw starting material supplied at the top of the furnace while gases circulate in such a way that there is a flow upwards with a counter-current flow of solid material which falls downwards. In order to simulate the reactions taking place in the furnace, it is necessary to take into account the fact that substances move in a temperature gradient during the process and that the temperature is controlled as much by the heat exchange and enthalpy of reactions as by external heating. Eriksson and Hack (1990) developed a module for the ChemSage software code which would help examine cases where there is material and heat flow as well as chemical reactions. This is achieved by conceptually separating up the furnace into a number of separate parts or 'stages' where local chemical equilibrium can be assumed. Flow is then modelled by including distribution coefficients between the stages. So, for example, in a reactor with two stages, material which reacts in one stage can move to another stage, dependent on the flow direction. The accuracy of the programme in dealing with dynamic flow, which is non-equilibrium in nature, lies in how many stages are used. The use of many stages will allow smooth changes to be considered but will cause a substantial increase in computational time. For the Si arc furnace four stages were considered and these are shown schematically below. GAS T *AH/kJ = 0 Stage 1 T T/K - 1784 i P/bar = 1.0 *AH/kJ = 0 Stage 2 T T/K = 2059 1 P/bar = 1.0 *AH/kJ = 0 Stage 3 T T/K = 2079 i P/bar = 1.0 *AH/kJ = 875 Stage 4 T T/K =» 2355 P/bar = 1.0 *regulated quantity j Input C SiOj (quartz) Condensed phases References are listed on pp. 402-408. 1784 K 1 20SS K 1 2079 K 2355 K V\CO(0) \ c \ SiO (G) -""SiC CO (G)SiC Siage «1 | Stage *2^ss | Stage »3 / Stage «4 \ TOP BOTTOM Figure 10.92 Flow scheme for various phases in a Si electric arc furnace (from Eriksson and Hack 1990). The raw materials, 1 mole of Si02 and 1.8 moles of C are introduced into the top stage where the temperature is 1784 K, while the energy from the arc, 875 kJ per mole of SiC>2, was taken to be released only in the bottom stage of the reactor. The reactor assumes each stage has fixed temperature and therefore the enthalpy input to the other three stages arises solely from heat exchange and reaction. The flow scheme (Fig. 10.92), distribution coefficients, values for the heat balances in each stage, input substances and initial temperatures are actually obtained by an optimisation process and relate to a particular furnace rather than genetically to all Si arc furnaces. The example above is from Eriksson and Hack (1990) but later calculations by the same authors (Eriksson and Hack 1996) give somewhat different results. However, the latter relate to a specific Si arc furnace at KemaNord, Ljungaverk, in Sweden. 10.6.8 Nuclear applications Nuclear applications constituted a strong area in the early stages of CALPHAD calculations, not only to obtain a better understanding of alloying in U- and Pu-based systems but also for handling complex gas reactions. The interest in applying CALPHAD to nuclear problems is well demonstrated by the papers of Potter and Rand (1980,1983) which reviewed work on a variety of problems, including simple calculations for the U-0 and U-Pt-0 systems, and more complex calculations for irradiated fuels and coolant reactions. Recently Ball et al. (1989,1996) have looked at the application of phase-equilibrium calculations to cladding failure in irradiated pins for water-cooled thermal and liquid-metal-cooled fast-breeder reactors and the analysis of accidents in nuclear reactors. 10.6.8.1 Cladding failure in oxide fuel pins of nuclear reactors. The long-term operational performance of nuclear fuel pins is critically governed by the reactions that occur in the gap between the fuel and its cladding. Ball et al. (1989) examined this for the cases of (1) Zircaloy-clad pellets of U02-t* in a pressurised water reactor (PWR) and (2) stainless-steel-clad pellets of (U, ?)02+x in a liquid-metal-cooled fast-breeder reactor (LMFBR). In particular they were interested in the influence of O potential on Cs, I, Te and Mo and the effects of irradiation on the gaseous species within the fuel-clad gaps. In the case of PWRs, which operate at relatively low centre temperatures (~1500 K), it was considered that little diffusion of fission product elements would occur to the gap, the majority of material in the gap arising from athermal processes such as fission-fragment recoil. The oxygen potential was taken to increase with increasing irradiation and a series of calculations were made at 650 K to predict the pressure of the predominant gas species as a function of oxygen potential. Two cases were considered: (1), Mo and Zr being zero, i.e., no presence of the fission-product Mo or interaction with the Zircaloy (Fig. 10.93(a)), and (2) with Mo and Zr included (Fig. 10.93(b)). Although qualitatively similar, the calculations show that the inclusion of Mo increased the I pressure in the gas due to the reaction of Csl with Mo-containing species to form CsjMoCV In LMBFRs, operating temperatures at the centre are nearer 2300 K, far higher than in PWRs, and the fuel is a mixture of U and P oxide (U, ¥)02+x- Any reactions must now include Cr from the oxide film of the stainless-steel cladding which has replaced Zircaloy. Figure 10.94(a) then show the calculated ratios of Te:Cs, I:Cs and Te:I for a reaction at 850 K, assuming that no fuel was involved in the reaction, which is then predominantly controlled by Mo and Cr, while Fig. 10.94(b) shows what happens when fuel is included, assuming similar levels of Mo and Cr. Again, the calculations show that predictions are qualitatively similar in both cases, but there are significant differences in the amounts of reaction. On the basis of the above calculations, Ball et al. (1989) concluded that, for PWRs, the potential of I in the gas from equilibrium reactions would be insufficient to account for stress corrosion cracking (SCC) of the Zircaloy. The inclusion of Mo, which can be present in the gap as a fission product, raised the iodine potential but, again, not to a level sufficient to account for any SCC. However, the concentrations of the elemental gaseous species could increase more significantly due to irradiation by fission fragments, and this may be sufficient to produce SCC of the Zircaloy. For the case of LMBFRs, I levels were also increased due to increased O potential. More importantly, Cs and Te levels would also be increased and, with the ratio Te:Cs>0.5, the calculations showed that these elements may deposit as solids onto the cladding surface leading to corrosion of the stainless-steel cladding. 10.6.8.2 Accident analysis during melt-down of a nuclear reactor. The problem to be considered here is the erosion of concrete by liquid material during a 'melt- References are listed on pp. 402-408. 396 7Y. Saunders and A. P. Miodownik 00 -10 - ' Pressure of I for SCC of Zircaloy „40 -700 (b) J_ -660 -620 -580 -S40 -500 -460 Oxygen potential / kJmol-1 -420 -3S0 cl. _20 - an o -25 - -700 -660 -620 -580 -540 -500 -460 -420 Oxygen potential / kJmol-1 Figure 10.93 Calculated pressures of the predominant gas phase species as a function of oxygen potential within the fuel-clad gap of a PWR fuel pin calculated for the case (a) where Mo and Zr are absent and (b) where Mo and Zr are included (Ball etal 1989). References are listed on pp. 402-408. CALPHAD—A Comprehensive Guide 397 (a) 12 4 - CO o l-J -8 -16 -20 -900 (b) 12 60 O -8 -12 -16 -20 -900 -700 -500 Oxygen poiential / kJmol-1 -300 Log (Te/I) Log (Tc/Cs) Log (I/Cs) -700 -500 Oxygen potential / kJmol-1 -300 Figure 10.94 Calculated ratios of amounts of Te:Cs, I:Cs and Te.I in the gas phase as a function of oxygen potential within the fuel-clad gap of a LMFBR fuel pin assuming (a) no fuel takes part in the reaction and (b) fuel is included in the reaction (Ball et al, 1989). down' of the reactor core. In this case the liquid core is 'relocated' into the bottom of the reactor vessel where immiscible oxide and metal liquids are formed. This is initially contained within a crucible of condensed material but, if the wall of the reactor pressure vessel is breached, the molten 'corium', comprising components of the core and structural materials, is ejected onto a concrete basemat in the secondary containment building. This concrete basemat is both thermally ablated and attacked by the molten 'corium-concrete' interaction (MCCI). In addition there are gas reactions which can potentially lead to the release of dangerous radioactive material into the atmosphere. To examine this problem more closely it was necessary to develop (1) a model for the nine-component oxide system U02~Zr02-SiO2-Ca0-Mg0-Al203-SrC^BaO-La203 to account for the MCCI (Chevalier 1992, Ball et al. 1993) and (2) develop a database for the gas-phase reactions in the oxide subsystem U02-ZrO2-SiO2-CaO-Mg0-Al203. The final oxide database included four solution phases and 70 condensed stoichiometric phases. Figures 10.95(a,b) show isopleths calculated between (a) corium and siliceous concrete and (b) corium and limestone concrete. Comparison between experimental (Roche et al. 1993) and calculated values for the solidus are in reasonable agreement, but two of the calculated liquidus values are substantially different. However, as the solidus temperature is more critical in the process, the calculations can clearly provide quite good-quality data for use in subsequent process simulations. Solidus values are critical factors in controlling the extent of crust formation between the melt-concrete and melt-atmosphere interface, which can lead to thermal insulation and so produce higher melt temperatures. Also the solidus, and proportions of liquid and solid as a function of temperature, are important input parameters into other software codes which model thermal hydraulic progression and viscosity of the melt (Cole et al. 1984). Calculations including the vapour phase were then made to determine the extent of release of various components during the reaction. Two types of calculation were made, one where ideal mixing in the solution phases was considered and the other where non-ideal interactions were taken into account. For elements such as Ba, U and, to a certain extent, Si, the calculations were relatively insensitive to the model adopted. However, the amount of Sr in the gas was 24 times higher in the 'full model' in comparison to the ideal model. This led to the conclusion that sensitivity analysis was necessary to determine the extent to which accuracy of the thermodynamic parameters used in the model affected the final outcome of the predictions. 10.6.8.3 The effect of radiation on the precipitation ofsilicides in Ni alloys. While chemical reactions in nuclear generators have dominated how CALPHAD methods have been used in practice for nuclear applications, there has also been a significant interest in the metallurgical aspects of materials under irradiation (Kaufman et al. References are listed on pp. 402-408. (a) Temperature — composition isopleth 3000 -S 2500 S 4» 2000 1500 PHASES 1 1 Liquid 2 Cubic 3 Tetragonal 4 Monocline 5 Melilite 6 Anorthile 7 Wollastonile 8 Pseudowollastonite 9 Alpha CaSi03 10 Alpha Prime CaSi03 11 Rankinite 12 CrisSobclite ^-v. 13 Tridymite 14 ZrSi04 — --—. Liquidus — — Soiidus f \ — 1+1+2+3 . /... . 1 + 1+2 1+1+2+12- -i + i+i*ui-> !+2+3+12 1+2+12+14 S^Tf^+^+U^^ ,+2+l3+,4 1+2+13'\ \2+3+6+8+14V^ J 1+2+8+13+14 - 2+4+\ 2+4+6 \ 6+14\ +7+14| \ 2+6+7+13+14 1 1 2+6+8+13+14 1 0.0 0.2 0.4 0.6 0-i Corium Proportion of concrete by moles Temperature - composition isopleth l.O Concrete 3000 2500 2000 1500 0.2 0.4 0.6 O.i Proportion of concrete by moles Figure 10.95 Calculated isopleths from 100% corium to 100% concrete, (a) For sicliceous concrete and (b) limestone concrete (Ball el al. 1996). 400 N. Saunders and A. P. Miodownik 1978, Miodownik et al. 1979, Watkin 1979). Irradiation can cause void-swelling, suppression of a formation in stainless steels and non-equilibrium precipitation of silicides. These phenomena are complex and occur by a combination of thermodynamic and kinetic effects. However, it was shown by Miodownik et al. (1979) that a thermodynamic analysis could be used to good effect to rationalise the effect of radiation on silicide formation. Although the work was done for a simple alloy system, it demonstrates how thermodynamics can be used in unusual circumstances. Barbu and Martin (1977) observed that increasing Ni+ dose rate enhanced the formation of Ni3Si in Ni-Si alloys (Fig. 10.96), causing it to form in 'sub-saturated' alloys whose Si levels were below the solvus composition for the formation of equilibrium Ni3Si. From a purely thermodynamic point of view an additional Gibbs energy (AG*) has to be taken into account which is shown schematically in Fig. 10.97. Miodownik et al. (1979) correlated this additional Gibbs energy to dose rate for sub-saturated Ni-Si alloys with 2 and 6at%Si (Fig. 10.98), and generated a diagram which showed how the formation of Ni3Si would occur in these alloys as a function of temperature and dose rate (Fig. 10.99). The diagram is analogous to a time-temperature-transformation diagram with the dose rate taking the place of the time axis. Rotating the axes also gives a form of diagram similar to that of Barbu and Martin (1977) shown in Fig. 10.96. Although the work was in the form of pseudo-equilibrium in the presence of irradiation, and did not take into account the effect of kinetics, it nevertheless gives a clear indication of an additional energy term due to irradiation. Similar studies were done by Kaufman et al. (1978) to show the magnitude of the Gibbs energy necessary to prevent a formation in Fe-Cr-Ni alloys. io- ta. 10" PRECIPITATION pptn OF Ni3Si _!_ 0 200 400 600 TEMPERATURE, °C Figure 10.96 Combinations of Ni* dose-rate and temperature leading to precipitation of Ni3Si (from Barbu and Martin 1977). References are listed on pp. 402-408. u os id z u \ COMPOSITION SHOWING \ /precipitation under \* irradiation conditions . ^ AG* = AGmax. gpcc NORMAL TANGENCY point ^ ■'